Quote Now

Printing on Metallised Film: Adhesion, White Underlay and Common Faults

Written by
Feng Yan
Last update:

By Feng Yan, Technical Engineer, CTPPressLast updated: November 2026Quick answer: When printing on metallized film,…

By Feng Yan, Technical Engineer, CTPPress

Last updated: November 2026

Quick answer: When printing on metallized film, first establish which surface you print on. If the metal is inside the structure, choose the ink for the outer film. Dyne test the plastic side, at least 36 mN/m for printing as typical practice. The metal shows through transparent inks, so use a white underlay or opaque ink where colours must look as on white. If ink and metal come off together, test the metal layer bond before you change the ink.

Key takeaways

  • Metallised film is plastic film or paper with a very thin aluminium layer. First establish which surface you print on.
  • If the metal layer is inside the structure, choose the ink for the outer film, not for the metal.
  • The metal shows through transparent inks. Where a colour must look as it does on white, print a white underlay or use an opaque ink.
  • When ink and metal come off together, the weak point is the bond between the metal and the film. Test the metal layer bond before you change the ink.
  • On arrival, check metal thickness, uniformity across the web, layer bond and pinholes.

The ink comes off with the tape and takes the metal with it. Or the ink does not stick to the metallised side at all. Or the colour looks different on the metallised film, darker and more metallic than the proof. Printing on metallized film (metallised film in British spelling) has its own faults, because the surface under the ink is not one simple material. This guide works through the print side, the surface, colour on metal, the metal layer and the common faults.

What metallised film is and which side you print

Metallised film is made in a high vacuum: aluminium vapour settles on a base film as a very thin layer. The result has a metallic shine and still bends like film. Common base materials are paper, PET, nylon, BOPP, CPP, LDPE, HDPE and cellophane. In flexible packaging it is used for its look and as a barrier layer in a laminate.

A common belief is that metallised film is always printed on the metal. Often it is not. First establish which surface you print on; if the metal layer is inside the structure, choose the ink for the outer film.

Structure Surface the ink meets Choose the ink for
Metal sandwiched between two films The outer, unmetallised film That film, for example OPP or PET
Clear film reverse printed, then laminated to metallised film The inside of the clear film, with the metal behind the print The clear film and the laminating adhesive
Metallised paper A special print coating over the metal That coating; ask the paper supplier
Metallised film printed on the metal side The metal, or a primer over it The metal or primer, with the ink supplier’s approval

Some metallised papers and metallised OPP need to be printed soon after metallising, because adhesion drops in storage. No single figure says how soon, so ask the supplier and use the oldest rolls first. Changing film, even to a “nearly identical” grade, means qualifying the ink again. Our flexible packaging printing page covers the plate side of film work.

Surface treatment and dyne level on the print side

On the plastic side of a metallised structure, the rules are the same as on any film. As typical practice, film needs at least 36 mN/m for printing and 38 mN/m for laminating. Many ink and adhesive suppliers ask for more, and their data sheet decides. See our dyne level test guide.

  • Storage. “The film supplier says the film is treated” describes the day the film was made. The level falls in storage, so test the roll again before the run. On PET, corona treatment also fades; ask which surface modification the film has.
  • Low readings on OPP. Slip and antiblock agents in OPP move to the surface and can give a misleading low reading. If an alcohol-based ink adheres normally on the same film, consider this before you add treatment.
  • In-line treatment. On metallised OPP, the metal surface can be given an in-line corona treatment on the press. Set the treater as its maker’s manual says. See corona treatment for film printing.
  • Back-side treatment. Keep the discharge off the reverse side. A treated back can stick in the roll, and it can ruin a cold seal on the back.
  • Primer and coating. A primer is a surface of its own. Ask its supplier which inks it takes.

Ink choice, white underlay and how the metal shows through

A metallised surface is like a mirror and takes up almost no ink, so the ink dries only by evaporation or by cure. Drying and cure settings matter as much as on plastic film; for UV inks see our UV flexo ink guide.

Many printers expect transparent inks to give the same colour on metallised film as on white film. They do not. The metal shows through transparent inks, so a white underlay or an opaque ink is needed where a colour must look as it does on white. Over bare metal the colour looks metallic, which designers use on purpose. Where the design needs a flat colour or a photo, the metal must be covered.

  • Where the white goes. The white must lie between the metal and the colour. On the metal side, the white goes down first and the colours go on top. When you reverse print clear film for lamination to metallised film, the colours go down first and the white after them.
  • Even white. Solid whites need even ink lay-down without pinholes, or the metal shows through in spots.
  • Barcodes. Metal reflects like a mirror, so a solid white panel behind the symbol is the usual answer; see bar width reduction for flexo barcodes.
  • Proofs. A proof on white stock will not show the colour you get on metal. For colours that match the proof on metallised film, proof on the same film with the same white.

Colour sequence on metallised paper. Common practice is to print small dark areas and tight-register colours first and a large background last, because a background printed first may not take the later colours and can be scratched in later units. The main colour tone goes late, because no ink is fully transparent and the hue leans towards the colour printed later. A white underlay under other colours is the exception, since it must go down first; then check that the next colours hold on it. If one colour does not hold on another, see ink trapping.

Checking the metal layer: optical density, uniformity, layer bond and pinholes

Metallised film is sensitive to moisture, so in principle packs are not opened for sampling. If you open one, reseal it at once and use the film soon.

Check How it is done Notes
Thickness by optical density Measure the light that passes through the film Not affected by surface oxidation. The reading depends on the instrument’s light, so record the instrument.
Thickness by sheet resistance Measure the electrical resistance of the metal layer Most accurate just after the roll comes off the metalliser, before the surface oxidises.
Visual check Lay two layers together and look at a lamp A rough estimate only. The eye adapts to dim light.
Uniformity Measure 8 to 10 samples of 100 mm × 100 mm, equally spaced across the web Give the average and the upper and lower deviation. A larger deviation means a less even layer.
Layer bond, tape test Press about 15 cm of 2.5 cm wide pressure-sensitive tape onto the metal. Pull it back at 180° at a steady speed, about 1 cm per second. Check tape and film on a light box for metal that has come off.
Layer bond, heat-seal peel For metallised PET: heat-seal a test film to the metal and peel it on a tensile tester Record the peel force and the metal transfer.
Pinholes and patches Look at the film against the light Points or areas where light passes through.

These methods give readings, not a pass or fail. Allowed deviation, metal transfer and peel force are set in your contract with the film supplier or in your own standard.

Common faults when printing on metallised film

“It must be the ink” is the first thought. When ink and metal come off together, the weak point is the bond between the metal and the film, so test the metal layer bond before you change the ink. Run the tape test on unprinted film from the same roll. If the metal comes off with no ink on it, the fault is in the film.

Symptom Likely cause Check or action
Ink comes off with the metal Weak bond between metal and base film Tape test unprinted film from the same roll; send results to the film supplier
Ink comes off, metal stays Surface not ready, wrong ink for the surface, ink not dry or cured Confirm the print surface, dyne test the plastic side, check the ink with its supplier, check drying or cure
Adhesion lower on old rolls Printed too long after metallising; treatment faded Use the oldest rolls first; test again before the run
Colour darker or more metallic than the proof Metal showing through transparent ink; no white or uneven white Add a white underlay or use opaque ink; proof on the same film
Scratches in a large background on metallised paper Background printed early, marked in later units Print the large background last where the design allows
Light points or patches in the metal Pinholes or thin areas in the metal layer Check against the light on arrival; measure uniformity

More press faults are in our flexo printing problems table.

Checklist before printing metallised film

  1. Establish which surface you print on and agree the ink for it with the ink supplier.
  2. Note the metallising date, use the oldest rolls first and keep packs sealed.
  3. Dyne test the plastic side. If you treat in line, keep the reverse side untreated.
  4. Check the metal layer: thickness, uniformity, tape test and pinholes.
  5. Decide where the white underlay goes and where the metal stays visible.
  6. Set the colour sequence and proof on the same film.

Record the treatment reading and metal layer results with each job, so a film fault is not counted against the ink or plate. We supply flexo plates for film work.

FAQ

Which side of metallised film do you print on?

It depends on the structure. If the metal is between two films, you print on the outer film and choose the ink for it. On metallised paper you print on the coating over the metal.

Why do you need a white underlay on metallised film?

The metal shows through transparent inks, so colours look darker and metallic. A white underlay or an opaque ink covers the metal where a colour must look as it does on white.

Why does the ink take the metal off with the tape?

The metal holds less well on the film than the ink holds on the metal. Tape test unprinted film from the same roll. If the metal comes off with no ink, the fault is in the film.

What dyne level does metallised film need for printing?

On the plastic side, typical practice is at least 36 mN/m for printing and 38 mN/m for laminating. Many suppliers ask for more, and their data sheet decides.

How do you test the metal layer on metallised film?

Measure thickness by optical density or sheet resistance, measure 8 to 10 samples across the web for uniformity, run a tape test for layer bond and look for pinholes against the light. Pass values come from your contract or your own standard.

Why does the colour look different on metallised film?

Light reflects from the metal through transparent inks, so the colour looks metallic. No ink is fully transparent, so the hue also leans towards the colour printed later.

Plates for a metallised film job? Request a plate sample with your film structure, ink system and plate thickness, or ask a technical question.

Disclaimer: the checks and values on this page are typical pressroom practice and for reference only. The ink, primer and treatment level for your job are subject to your film, ink and adhesive suppliers’ data sheets, and metal layer pass values are set in your contract.

About Feng Yan

Feng Yan is a technical engineer at CTPPress with more than 20 years in the printing industry and extensive front-line experience supporting printing plants. Feng specialises in solving the difficult problems printers run into in production.

Talk With Author >>

Start Your Business With Us

Simple Contact Form

Tell us what you need

Request a Quote

Tell us which printing plates or equipment you need, including specifications, quantity and destination. Use the form to send your enquiry.

Aluminium coils and printing plate production equipment
Product Enquiry

Request an Instant Quote

We reply within 24 hours on working days

Product Enquiry
Aluminium coil on an offset plate production line