Last updated: November 2026
Quick answer: UV flexo ink does not dry: UV light starts a reaction in the photoinitiator and the ink becomes a solid film. When it stays tacky, check the curing unit first: lamp hours, reflector, electrics and cooling air, then dose, ink film, distance and speed. The depth of cure depends mainly on irradiance, so a lamp short on power will not cure the ink through, however slow the press runs.
Key takeaways
- UV flexo ink does not dry. UV light starts a reaction and the ink becomes a solid film, so you judge it by cure.
- The depth of cure depends mainly on irradiance, not on time. A lamp that is short on power will not cure the ink through, however slow the press runs.
- Dose is irradiance multiplied by time: E = I × t. Run production at about 0.8 times the speed at which the ink just fails to cure.
- Check the curing unit before you blame the ink: lamp, reflector, electrics and cooling air first.
- Plates and rollers must resist the UV ink and the UV wash.
The UV ink is still tacky after the lamp. Or the surface is cured but the ink underneath is still soft. On film labels the ink comes off with tape, the print sets off on the back of the next layer in the roll, or thin film shrinks or distorts under the lamp. These faults usually start in the curing unit, not in the ink. This guide explains how UV curing works and how to find the cause in a fixed order. Its lamp values are for mercury and metal-halide lamps; LED-UV curing works differently and is outside this guide.
How UV flexo ink cures
Water-based and solvent-based inks dry when their water or solvent evaporates. See solvent vs water-based flexo ink. UV ink has nothing to evaporate. It contains oligomers (the resin), monomers (which set the viscosity) and photoinitiators. When UV light reaches the photoinitiator, it starts a chain reaction, and the monomers and oligomers link into a solid film. The monomers do not evaporate; they stay in the film.
Many printers say that UV ink “dries like other flexo inks”. It does not dry. Light starts a reaction, so you judge UV ink by cure, and you need one agreed cure test in the pressroom.
- Free radical (acrylic) UV ink: oxygen in the air slows the reaction, so the ink maker adds a co-initiator.
- Cationic UV ink: oxygen does not slow it and it adheres well to film, but amines stop the cure. It cannot be used on substrates or with pigments that contain amines.
What UV ink changes at the press
- No drying on the plate or in the anilox. The ink only cures under UV light, so dots do not bridge between impressions.
- Stable viscosity. Nothing evaporates, so viscosity changes little during the run. Adding solvent does not apply, because the monomer is not a solvent.
- Judged by cure. A print can feel dry on the surface and still be soft underneath.
- Black is the hardest colour to cure. Giving every colour the same energy can leave the black under-cured.
- Handling. Avoid skin contact, and do not clean UV ink off the skin with solvent.
Plates and rollers. UV ink and UV wash can swell a photopolymer plate that is not made for them. The usual choice is a UV-resistant solvent-washout plate grade; use a thermal-processing plate only if the grade is rated for UV ink, and do not use water-wash plates. See flexo ink and plate compatibility and printing plates for UV ink. Rubber rollers must resist both the UV ink and the UV wash. EPDM is the usual compound for UV ink, and a standard nitrile roller is not suited to it; see EPDM vs nitrile rollers.
The parts of the UV curing unit that decide the result
If a lamp goes dark, flickers or will not start, or the power supply overheats, that is a hardware fault: fix it first, then come back to cure. With the hardware in order, use this simple check list for the curing unit.
| Part | What to check | Sign of a problem |
|---|---|---|
| Lamp | Hours against rated life, typically about 800 to 1,000 hours for mercury lamps (the lamp maker’s data decides). Clean lamp and reflector with anhydrous alcohol as dust requires; turn the lamp 90° when you clean it. | Cure gets worse slowly as the lamp ages |
| Reflector | Aluminium, semicircular, lamp at the focus. Not iron or stainless steel, which darken in the heat. | A missing or unsuitable reflector wastes about 40 to 50% of the UV energy; more lamp power does not solve this |
| Transformer and capacitor | Output matched to the lamp power; capacitor rating matched to the transformer | Too high a voltage burns lamps; too low gives too little power |
| Cooling air | Adjustable supply and extraction fans; air never blown straight onto the lamp | Light turns from white to blue: too much cooling. Hot housing or a warped lamp: too little |
| Control | Fans run after switch-off until lamp and housing are cool; restart a lamp only when fully cool | Short lamp life |
| Housing | Flat surfaces, guarded hot areas, no light leaks | Light escaping from the unit |
Dose, irradiance and press speed
Irradiance (I) is the UV power reaching each square centimetre, in mW/cm². Dose (E) is the UV energy delivered: E (mJ/cm²) = I (mW/cm²) × t (s). At the same irradiance, a faster web spends less time under the lamp, so the dose falls in proportion to the speed.
When UV ink stays tacky, the first idea is often “just run the press slower” or pass it under the lamp again. The depth of cure depends mainly on irradiance, not on time. A lamp that is short on power will not cure the ink through, however slow the press runs. The extra light ages the surface, makes it brittle and reduces adhesion. Confirm lamp power, reflector and cooling first, and slow the press only when the irradiance is right and the dose is still short.
“More UV energy is always safer” is another belief to correct. The dose only needs to be slightly above what the ink needs, and the ink maker states that value. Overdosing wastes energy and can damage the cure.
The speed test. On a press with mercury or metal-halide lamps, this test gives a press speed that cures every time:
- Start at a speed at which the ink cures.
- Raise the speed step by step, checking with your agreed cure test.
- Note the speed at which the ink just fails to cure (vc).
- Run production at 0.8 × vc.
- Repeat after a lamp change and as lamp hours build up.
A UV radiometer measures irradiance, dose and temperature. Log its readings next to your cure results and use the log to decide when to change lamps or speed.
Why UV ink stays tacky or does not adhere
How to check cure. Choose one test, for example a thumb press, a solvent rub or a tape test. Write down how it is done and use it at the same point every time. A cure test the whole crew uses makes results from different shifts comparable.
The common symptoms are a tacky surface, a surface cured but not through (poor through cure), poor adhesion and set-off in the roll. It is tempting to say “the ink must be bad”. Check the causes in this order instead:
- Hardware: rule out lamp and power supply faults.
- Irradiance: every item in the curing unit table in order.
- Dose: E = I × t against the ink maker’s value.
- Ink film: too thick cures slowly and heats the substrate.
- Lamp distance: too close distorts the substrate, too far leaves the surface tacky. Use the curing unit maker’s setting.
- Speed: too fast leaves the ink cured on the surface but not through; too slow ages the substrate.
- Heat and cooling: see the next section.
- Pressroom: about 15 to 25 °C, out of direct sunlight.
Poor adhesion can also come from a surface made brittle by a slow press, or from the substrate. Ink only adheres to a film whose surface is treated well enough, so measure it with a dyne level test. Some label facestocks need a topcoat before they take a given ink; see label printing.
Set-off in the roll happens when ink that is not cured through is rewound and transfers to the back of the next layer. Fix the cure first.
Heat on thin film
A mercury lamp turns about 60% of its power into infrared, and the lamp surface runs at about 700 to 800 °C. Thin film takes up this heat and can shrink or distort. Air cooling is the most common control. A water-cooled jacket works well but costs more. An infrared-blocking filter suits products that distort easily.
Balance the cooling. Too little distorts the substrate and shortens lamp life. Too much keeps the lamp from reaching full power, and the ink then does not cure. A slow press, a lamp set too close and a thick ink film all add heat, so check them first.
UV flexo ink troubleshooting table
| Symptom | Likely cause | Check or fix |
|---|---|---|
| UV ink still tacky after the lamp | Low irradiance or dose, lamp too far, air on the lamp | Check lamp hours, reflector, air flow; measure; repeat the speed test |
| Surface cured, soft underneath | Speed too high, ink film too thick, lamp short on power | Fix lamp power first; then reduce speed or ink film |
| Black under-cured | Black needs more energy | Ask the ink maker for the dose for black |
| Ink comes off with tape on film | Low surface treatment, no topcoat, under-cure or brittle surface | Dyne test the film; check the facestock and the cure |
| Cationic ink does not cure on one substrate | Amines in the substrate or pigment | Change the substrate or the ink system |
| Set-off in the roll | Ink not cured through before rewinding | Fix the cure |
| Film shrinks or distorts | Infrared heat, slow speed, lamp too close, too little cooling | Improve cooling or fit an infrared filter |
| Dots grow during the run | Plate not rated for UV ink | Use a UV-resistant solvent-washout grade |
For other press faults, see flexo printing problems. For plate types, see our flexo plates range.
FAQ
Why is my UV ink still tacky after curing?
Usually the irradiance or the dose is too low. Check lamp hours, reflector, cooling air and lamp distance, then speed and ink film.
How does UV flexo ink cure?
UV light starts a reaction in the photoinitiator, and the monomers and oligomers link into a solid film. Nothing evaporates, so you judge it by cure, not by drying.
Can you slow the press down to cure UV ink better?
Only when the irradiance is right and the dose is short. If the lamp is short on power, a slower press ages the surface instead of curing the ink through.
How do you check if UV ink is fully cured?
Use one agreed test, such as a thumb press, a solvent rub or a tape test, the same way every time, and log radiometer readings next to the results.
Why does UV ink have poor adhesion?
Under-cure, a brittle surface from a slow press, a film surface that is not treated well enough, or a facestock without a suitable topcoat.
Which plates and rollers suit UV flexo ink?
A UV-resistant solvent-washout plate grade, or a thermal grade only if rated for UV ink; not water-wash plates. EPDM is the usual roller compound.
Setting up UV flexo work? Request a quote for flexo plates with your press, plate gauge, ink system and wash, or ask a technical question.
Disclaimer: the checks and values on this page are general pressroom practice and for reference only. Lamp values apply to mercury and metal-halide lamps, not to LED-UV. The dose your ink needs is set by the ink maker’s data sheet, and lamp settings by the curing unit maker’s manual.