Last updated: November 2026
Quick answer: A dyne test checks whether the surface of a plastic film can be wetted by ink or adhesive. Spread a test liquid of known wetting tension over about 6 cm² of film and watch it for 2 seconds. The reading is the highest liquid that stays as an unbroken film. As typical practice, film needs at least 36 mN/m for printing and 38 mN/m for laminating. The level falls in storage, so test again before the roll goes on the press.
Key takeaways
- Dyne level is the wetting tension of the film surface, in mN/m. Ink and adhesive only spread and bond when it is high enough.
- Untreated polyethylene is at about 31 mN/m. As typical practice, film needs at least 36 mN/m for printing and 38 mN/m for laminating.
- Spread a test liquid over about 6 cm² of film and watch it for 2 seconds. The reading is the highest liquid that stays as an unbroken film.
- The level falls in storage, faster in a warm store. Test again before the roll goes on the press.
- If the dyne level is fine and the ink still lifts, look at the ink and the process.
The ink does not stick to the film. The print looks fine at the rewind, then the ink comes off with tape, or the laminate pulls apart. The film supplier says the film is corona treated. The ink supplier says the ink is right. A dyne test is the quick test that tells you which side to look at, before the roll goes on the press. This guide explains how to run it, what dyne level the film needs for printing and laminating, and what to do when the reading is fine but adhesion is still poor.
What dyne level means
Dyne level is the pressroom name for the wetting tension of a film surface. It is also called the surface tension of film, or its surface energy. It is given in millinewtons per metre (mN/m). One dyne per centimetre is the same as one mN/m, so a film “at 38 dynes” has a wetting tension of 38 mN/m.
On a film with a high dyne level, ink and adhesive spread into an even layer. On a film with a low dyne level, they pull back into drops. A dyne test does not measure ink adhesion. It measures whether the surface can be wetted. Good wetting is needed for adhesion, but it is not the only condition.
Why untreated polyolefin film does not hold ink
Polyethylene (PE) and polypropylene (PP) are low-polarity plastics. An untreated polyolefin film has almost no chemical groups at its surface that an ink or an adhesive can hold on to, and its surface energy is low. Untreated PE is at about 31 mN/m. That is below the level printing needs, so the ink does not spread evenly and does not bond.
Corona treatment raises the level. Our guide to corona treatment for film printing explains what decides it. An electrical discharge adds oxygen-containing polar groups to the film surface, and the surface tension goes up. Film is treated in this way before printing, laminating, coating, metallising and hot stamping. The dyne level you measure is the result of that treatment, and it changes with time.
How to run a dyne test with test liquids or pens
Test liquids are mixtures made to a known wetting tension. A common set is based on formamide and ethylene glycol monoethyl ether and runs from 30 to 56 mN/m. Buy them ready-made, with the value marked on each bottle. They are hazardous chemicals, so follow the supplier’s safety data sheet.
- Use standard conditions. Test at about 23 ± 2 °C and 50 ± 5% relative humidity.
- Take a clean sample. Take it from below the outer wraps of the roll, across the full web width. Do not touch the test area. Mark the treated side.
- Apply the liquid. With a clean cotton swab, spread one test liquid over about 6 cm² of film. Use a new swab for each liquid.
- Read at 2 seconds. If the liquid film stays whole for 2 seconds, the film is at or above the value of that liquid. If it breaks into drops within 2 seconds, the film is lower.
- Step up or down. Move to the next liquid on a fresh area. The reading is the highest liquid that stays unbroken for 2 seconds. If the top liquid of the set, 56 mN/m, still holds, record “56 or above”.
- Record it. Write down the film type, the side, the reading, the first liquid that broke, the room temperature and humidity, and the date. If the edges and the centre of the web differ, judge the roll by the lowest position.
Temperature and humidity. A reading taken in a hot, cold, dry or damp room can differ from a reading at standard conditions. If the reading is at or next to the level you need and the room was far from standard conditions, do not accept or reject the roll on it. Repeat the test at standard conditions.
Dyne pens. A dyne pen holds a test liquid of one value in a felt tip. Draw a line across the film and read it in the same way: the line stays whole, or it breaks into drops. A pen is fast, but it has two weak points. The tip touches the film, so it can carry slip agent and dirt to the next test. And one pen only says pass or fail at one value. When the result decides whether a roll is used, use test liquids with fresh swabs.
What dyne level film needs before printing and laminating
| Film and job | Typical minimum level |
|---|---|
| Printing on corona-treated PE or PP film | 36 mN/m |
| Laminating | 38 mN/m |
| Printing on the treated side of BOPET film | 52 mN/m |
| Coating, metallising, hot stamping | Treatment is needed, but there is no single figure. Ask the film or coating supplier. |
These are typical practice values, not the requirement of a standard. Many ink and adhesive suppliers ask for more than these minimums, and water-based inks usually need more than solvent-based inks. Follow the supplier’s data sheet when it gives a figure. A reading that is exactly on the minimum passes, but it is at the lower limit, with no margin for any fall in storage.
A common belief is that a higher dyne level is always better. It is not. The reading only needs to pass the level for the job. Film that is treated for too long can age at the surface, pick up an odour, stick at the roll edges and lose gloss. Film that is treated too hot can form a weak layer at the surface. The dyne reading then goes up while the bond strength goes down.
Why the dyne level falls in storage
“The film is corona treated, so it is ready to print” is the belief that causes the most surprises. The treatment level falls in storage, so test the film again before it goes on the press. A film that was treated and passed at delivery can give a reading that is too low now.
- The first days are the fastest. The level drops most quickly just after treatment.
- Heat speeds it up. In one reported storage test, treated PP and PE films kept at 28 °C fell below 38 mN/m in about 40 days. The same films kept at 10 °C fell only slowly.
- After a month. After more than a month, most PP and PE grades have fallen back to about 38 mN/m. Kept below 20 °C, cast film can hold 38 to 41 mN/m for at least a month.
- Additives move. Slip agents, antioxidants and antistatic agents migrate to the film surface and form a weak layer between film and ink. Films with a high additive content, and thicker films, lose their level faster.
Store film cool, use the oldest rolls first, and test every roll that has been stored for a long time or through a hot season. No single figure says how many days a film may be stored.
What to check when the reading is too low
A low reading means the surface is not ready. More ink, a stronger solvent or more impression will not correct it. Find the cause first.
| What you find | Likely cause | Check or action |
|---|---|---|
| The roll passed at delivery and is low now | The level has fallen in storage | Check the treatment date and the store temperature. Ask the film supplier whether the film can be treated again. |
| A newly delivered roll is low | Weak treatment at the film maker, or old stock | Test several rolls. Send the supplier your readings and test conditions. |
| The reading is very low over the whole web | You are testing the untreated side | Test both sides and mark the treated one. |
| In-line treater: low after the line speed was raised or a thicker film was run | Less treatment for each area of film; thicker film needs more energy | Raise the treater output as the treater maker’s manual allows, and test again. |
| In-line treater: low in damp weather | High humidity weakens the treatment | Improve the extraction of damp air around the electrode. |
After any change, run the dyne test again.
Dyne level fine but adhesion still poor
Poor ink adhesion on film does not always mean the dyne level is too low. When the reading passes and adhesion is still poor, it is an ink or process question. “The dyne pen says it is fine, so it must be the ink” may be right, but check the press as well. These points show if the problem is the film, the ink or the process.
- Ink system. Confirm with the ink supplier that the ink is made for this film and this end use. See flexo ink and plate compatibility for the ink systems in brief.
- Drying. Ink that is not fully dry, or that still holds solvent, does not bond well. A heavy ink film dries slowly, and the ink volume is set by the anilox; see the anilox roller guide.
- A weak surface layer. A film can read high and still bond badly when slip additive has migrated to the surface or when the film was over-treated. This is a possibility to test with the film supplier, not a conclusion.
- Ink on ink. If the first colour holds on the film but the next colour does not hold on the first, the fault is in the ink trapping, not in the film.
- Pinholes in solids. These are also a wetting fault, and the cause can be on the ink side. See flexo pinholing.
More press faults are in our flexo printing problems table. We supply flexo plates for film work; see flexible packaging printing for the plate side. For metallised structures, see printing on metallised film. When you trial a new plate on film, record the dyne level of the film, so that a film fault is not counted against the plate. Our plate test protocol lists what else to record.
FAQ
What is a dyne test?
A dyne test checks whether the surface of a plastic film can be wetted by ink or adhesive. A test liquid of known wetting tension is spread on the film. If it stays unbroken for 2 seconds, the film is at or above the value of that liquid.
What dyne level is needed for printing on film?
As typical practice, corona-treated PE and PP film needs at least 36 mN/m for printing and 38 mN/m for laminating. The treated side of BOPET film is usually specified at 52 mN/m or above.
How do you use a dyne pen?
Draw a line across the film. If the line stays whole, the film is at or above the value of the pen. If it breaks into drops, the film is lower. Use test liquids when the result decides whether a roll is used.
Is dyne level the same as surface tension?
In the pressroom, yes. Dyne level, wetting tension and surface tension of film are used for the same reading. One dyne per centimetre is the same as one mN/m.
Why does the dyne level of film drop in storage?
The level from corona treatment falls with time, fastest in the first days and faster in a warm store. After more than a month, most PP and PE grades have fallen back to about 38 mN/m.
What should I check when the dyne level is fine but the ink still comes off?
Then it is an ink or process question. Check that the ink system suits the film and that the ink is fully dry. Ask the film supplier about slip additive and over-treatment, because a film can read high and still bond badly.
Testing a new plate on film? Request a plate sample with your ink system, film type and plate thickness, or ask a technical question.
Disclaimer: the levels and checks on this page are typical pressroom practice and for reference only. The level your job needs is subject to the data sheets of your film, ink and adhesive suppliers.