Last updated: November 2026
Quick answer: Corona treatment passes plastic film through an electrical discharge. The discharge adds oxygen-containing polar groups to the film surface, so ink and adhesive can wet it and bond. Film is treated at the film maker and often again in line on the press or laminator. The level depends on treater output, line speed, film thickness, electrode gap, the treater roll covering, humidity and the additives in the film, and it fades in storage. Measure it with a dyne test before the job.
Key takeaways
- Corona treatment adds oxygen-containing polar groups to a low-polarity film surface, so ink and adhesive can wet it and bond.
- Film is treated at the film maker, and often again in line on the press or laminator. The level you print on is what is left on the day.
- The treatment level depends on treater output, line speed, film thickness, the electrode gap and condition, the treater roll covering, film temperature, humidity and the additives in the film.
- More output is not always better. Above a certain output the gain is small, and over-treatment can lower the bond strength.
- On an under-treated web, confirm the reading and check storage first, then the treater.
The film is sold as corona treated, but the ink holds in some bands across the web and lifts in others. Or the adhesion was good last month and is weak now, with the same film, the same ink and the same treater setting. You raised the treater power and the adhesion did not improve. Corona treatment is the usual surface treatment before printing on plastic film, and its result depends on much more than the power setting. This guide explains what the treatment does, what decides the level, what goes wrong with too little and too much, and what to check on an under-treated web.
What corona treatment does to a polyolefin film surface
Polyethylene (PE) and polypropylene (PP) are low-polarity plastics. An untreated polyolefin film has a low surface energy, so ink and adhesive do not spread on it and do not bond. Untreated PE is at about 31 mN/m.
In a corona treater, the film runs over a treater roll and passes under an electrode. A high-voltage, high-frequency discharge crosses the air gap between the electrode and the film. The discharge adds oxygen-containing polar groups to the film surface, and the surface tension goes up. Corona treatment of film is done in this way before printing, laminating, coating, metallising and hot stamping.
The result is measured as a dyne level, in mN/m. As typical practice, film needs at least 36 mN/m for printing and 38 mN/m for laminating. Many ink and adhesive suppliers ask for more, and their data sheet decides. The test itself is in our dyne level test guide. Run it before you change anything on the treater.
Where film is corona treated: at the film maker and in line
- At the film maker. Film is treated on the extrusion line, soon after it is formed. Warm film takes the treatment better than cold film, so the electrode is normally placed after the film has set and before it has cooled down. This is the corona treated film you buy, treated on one side or on both.
- In line on the press or laminator. Many film presses and laminators have their own corona treater before the first print unit or the adhesive station. It raises the level again just before the ink or adhesive goes on.
Use an in-line treater as a refresh for film that was treated at the film maker. Whether it can treat a film that was never treated is a question for the film supplier and the treater maker.
“The film is already corona treated by the supplier” describes the day the film was made. It is also a common belief that the same treater setting gives the same treatment level. It does not. The level you print on is what is left on the day, so measure it on the web before the job.
What decides the treatment level
Many printers believe that weak ink adhesion means the treater power is too low, so more power will fix it. Output is one factor of several. Line speed, film thickness, the electrode gap, the treater roll covering, humidity and additives all change the level, and above a certain output the gain is small.
| Factor | How it changes the level |
|---|---|
| Output power or current | Too little output gives a weak treatment. Above a certain value, more output adds very little. The best output for a film is found by trial, with a dyne test after each step. |
| Line speed | A faster line gives each area of film less time under the electrode, so it needs more output. |
| Film thickness | A thicker film needs more energy for the same level. |
| Electrode gap and condition | A gap that is too wide loses energy. A gap that is not the same across the web gives a level that is not the same across the web. Set the electrode gap as the treater maker’s manual says. |
| Treater roll covering | An aged sleeve, or one with bubbles, impurities or uneven wall thickness, gives a weak or uneven treatment. |
| Film temperature | Warm film takes the treatment better than cold film. This is used at the film maker. Too much heat is a risk; see over-treatment below. |
| Humidity | High humidity weakens the treatment and makes electrical breakdown at the treater more likely. The extraction must remove damp air from around the electrode. |
| Polymer | PP needs more energy than PE. For PE, a higher density is harder to treat, up to a certain density. |
| Additives in the film | Slip agents, antioxidants and antistatic agents move to the film surface and form a weak layer under the ink. Film with many additives is harder to treat. |
No single setting suits every job. The right output for one film, at one speed, on one treater does not carry over to another.
Signs of under-treatment and risks of over-treatment
Under-treatment. On film with too low a level, the ink does not wet the surface evenly and the ink adhesion is weak:
- The ink pulls back and leaves pinholes in solids.
- The dry ink comes off in a tape test.
- The laminate has a low bond strength.
- The fault runs in bands along the web, always at the same position across the width. This points to a treater, at the film maker or in line, where the electrode or the roll covering is not even.
- The fault covers the whole web. This points to output, speed or storage.
More ink, a stronger solvent or more impression will not correct an under-treated surface.
Over-treatment. “A higher treatment level is always safer” is a costly belief. Over-treatment can age the surface and form a weak layer, so the reading goes up while the bond strength goes down.
- Film that is treated for too long can age at the surface, pick up an odour, stick at the roll edges and lose gloss.
- Film that is treated too hot can form a new weak layer at the surface. The dyne level rises, but the bond is weaker.
No single figure marks where over-treatment starts. When a film reads high and still bonds badly, over-treatment is one possibility to check with the film supplier. It is not a conclusion.
Back-side treatment
Back-side treatment means that the side of the film that should stay untreated has also been treated. It can happen when air is trapped between the film and the treater roll, for example at a wrinkle or where the film does not lie flat on the roll. The discharge then also reaches the reverse side.
In the roll, a treated face then lies against a treated back, and the layers can stick together. Ink can also stick to the reverse side in the rewind. On a film that is sealed later, the sealing side may behave differently.
To find it, test both sides of the film. The side that should be untreated should read like untreated film. If it reads high in places, check the web for wrinkles and check how the film lies on the treater roll.
Why the treatment level fades
The treatment level is highest just after treatment and then falls. It falls fastest in the first days and faster in a warm store. Additives explain part of it: they keep moving to the surface after treatment. Film with many additives, and thicker film, fade more.
After more than a month, most PP and PE grades have fallen back to about 38 mN/m. The storage figures are in the dyne test article.
Store film cool, use the oldest rolls first, and test again before the roll goes on the press.
Checklist for an under-treated web
This is a practical order that starts with the checks that cost least. It is not a rule. After each change, test the film again.
| Step | Check | Action |
|---|---|---|
| 1. The reading | The treated side was tested, at the edges and the centre. | Repeat the dyne test. Note where across the web the level is low. |
| 2. Storage | The treatment date and the store temperature. | Refresh faded film on the in-line treater, or ask the film supplier. |
| 3. Output | The output, against the last good run. | Raise it in steps and test after each. When a step gives no gain, stop. |
| 4. Line speed and film thickness | A faster line or a thicker film than on the last good run. | Give more output for a faster line or a thicker film. |
| 5. Electrode | The gap is correct and the same across the web. The electrode is clean. | Reset and clean it as the treater maker’s manual says. |
| 6. Treater roll | A covering that is aged, has bubbles or is uneven. | Replace the covering. |
| 7. Humidity | Damp air, and whether the extraction works. | Remove damp air from around the electrode. |
| 8. Film | A change of grade, polymer or additives. | Send the film supplier your readings and test conditions. |
If the level passes across the full web width and the ink still lifts, the cause is in the ink or the process. See flexo ink and plate compatibility for the ink system, ink trapping if one colour does not hold on another, and our flexo printing problems table for other press faults. We supply flexo plates for film work; see flexible packaging printing for the plate side.
FAQ
What is corona treatment of film?
Corona treatment passes plastic film through an electrical discharge. The discharge adds oxygen-containing polar groups to the film surface and raises its surface tension, so ink and adhesive can wet the film and bond.
Why is corona treatment needed before printing?
PE and PP are low-polarity plastics with a low surface energy. Untreated PE is at about 31 mN/m, and as typical practice film needs at least 36 mN/m for printing.
How long does corona treatment last on film?
No single figure applies. The level falls fastest in the first days and faster in a warm store, and film with many additives fades more. Test the film again before the roll goes on the press.
Can film be over-treated with corona?
Yes. Film treated for too long can age at the surface, pick up an odour, stick at the roll edges and lose gloss. Film treated too hot can form a weak layer, so the dyne level goes up while the bond strength goes down.
What is back-side treatment on corona treated film?
It is treatment on the side that should stay untreated. It can happen when air is trapped between the film and the treater roll. Test both sides of the film to find it.
Why is ink adhesion uneven across corona treated film?
A fault in bands along the web, always at the same position across the width, points to a treater, at the film maker or in line, where the electrode or the roll covering is not even. Test the level at the edges and the centre.
Testing a new plate on film? Request a plate sample with your ink system, film type and plate thickness, or ask a technical question.
Disclaimer: the levels and checks on this page are typical pressroom practice and for reference only. Treater settings are subject to the treater maker’s manual, and the level your job needs is subject to the data sheets of your film, ink and adhesive suppliers.