Quote Now

Washboarding and Other Corrugated Board Print Defects

Written by
Feng Yan
Last update:

By Feng Yan, Technical Engineer, CTPPressLast updated: November 2026Quick answer: Washboarding is the flute pattern…

By Feng Yan, Technical Engineer, CTPPress

Last updated: November 2026

Quick answer: Washboarding is the flute pattern showing in a corrugated print: stripes in solids and tints that follow the flutes, because the liner is not flat over them and the plate prints harder on the flute tips. More pressure does not cure it; it crushes the board and lowers its strength. Check the liner, flutes and board temperature first, then print at kiss impression with a softer plate and a cushion behind it.

Key takeaways

  • Washboarding is the flute pattern showing in the print: stripes in the solids that follow the flutes, because the liner is not flat over the flutes.
  • More printing pressure does not cure it. It crushes the board, lowers its caliper and flat crush strength, and the print gets worse.
  • Many corrugated board print defects start in the board itself: uneven or collapsed flutes, caliper that varies in the lot, short blanks and warp.
  • Board straight off the corrugator is warm and moist. Let it reach room temperature before you print it.
  • Check each new lot before it goes into the feeder, and use a softer, thicker plate with a cushion behind it rather than extra squeeze.

You see stripes in the solids that follow the flutes. The operator adds impression and the stripes fade a little, but, as many printers put it, “the board crushes when we add pressure”. Or the short blanks skew, jam and do not glue at the folder gluer. These are common corrugated board print defects in postprint flexo, and most of them do not start on the press. This guide covers the causes in the board and on the press, the other board defects, plate choice and what to check on incoming board.

What washboarding is and why it shows in solids

Corrugated board is a liner glued over a fluted medium. The liner is supported at the flute tips and less so between them, so its surface is not flat. The plate presses harder on the flute tips and more lightly in the valleys. Ink transfer follows that pattern, and the print shows light and dark bands that run with the flutes. Printers call this washboarding, the washboard effect or fluting.

The fault shows most in solids and tints. A large, even area of one colour makes every small change in ink transfer visible, and the eye picks up a regular pattern at once. Text and line work break the pattern up.

Washboarding is different from flute crush. In washboarding the board is whole and the stripes are in the ink. In flute crush the flutes are flattened and the box loses strength. The usual reaction to the first fault causes the second.

Board-side causes of washboarding

The main cause sits in the board. The liner is not flat over the flutes, and the press can only print the surface it is given.

  • Light liner. The lighter the liner, the more easily washboarding appears. See the board conditions below.
  • Flute size. Fine flutes such as F, N and micro flutes give a smoother printing surface and can carry finer images than coarse flutes.
  • Flute structure. Flutes that lean, differ in height or have collapsed leave low spots in the liner that take less ink.
  • Liner surface. A rough surface, loose fibres and dust make the solid look patchy on top of any flute pattern.

Because these causes are in the board, the fix is mostly at the board plant. Record the lot number and send samples of the striped print to the supplier.

Press-side causes: impression, feeding and warm board

A common belief is that more printing pressure will fill in the washboard stripes. More pressure crushes the board and lowers its flat crush strength, so washboarding is solved at the board and the plate, not with pressure. The board gets thinner, the box gets weaker and the print quality falls as well. Corrugated postprint works at a light kiss impression: just enough to print the solid.

  • Impression. Set the plate to the board at kiss impression. If the stripes only disappear when the board is crushed, the cure lies in the board or the plate build.
  • Feeding. Set the feed gate to the caliper of the lot, neither tight nor loose, with light pressure from the feed rolls or belts. Too much pressure leaves embossed marks and crushes good flutes before the sheet is printed.
  • Warm board. Board straight off the corrugator is warm and moist. It changes ink transfer and drying, and it shrinks as it cools.

A heavy ink film on solids can make banding more visible, so check the anilox and ink too; see our anilox roller guide.

Other corrugated board print defects

Washboarding is one of five board defects an operator should recognise before the board goes into the machine. Checking first avoids waste and downtime.

Board defect What you see Effect on print and converting
Flute structure: leaning, uneven height or collapsed flutes Soft or sunken areas in the liner Low flat crush strength; sunken areas are hard to print; printing hard into them crushes the good flutes around them
Caliper that varies within the lot Sheets or bundles of different thickness Double feeds when the gate is set for thin board; skew when guiding force is too low; embossed marks and crushed board where it is thick
Washboarding Flute lines visible in the liner, worse on light liners Stripes in solids and tints that follow the flutes
Blank length: too long or too short Blanks that do not match the job size Long blanks waste board; short blanks skew, jam and the glue flap does not reach the side panel
Warp Sheets bowed up or down, end to end, S-shaped or twisted Feeding and print problems; the press has to work around it

Crushed board. Some board arrives with collapsed flutes. Other board is crushed on the press by extra impression or heavy feed roll pressure. Compare the board before and after the print unit to see where it happens.

Short blanks. Either the blanks were cut short at the corrugator, or warm, moist board shrank as it cooled. Let the board reach room temperature in the press hall and measure again before you decide.

Warp, surface pH and stiffness. Warp, a change in the liner’s surface pH and board that is too stiff have no standard press-side correction. Note the lot and report it to the board supplier.

How plate choice affects corrugated print defects

The plate cannot make a bad board flat, but it decides how well the print copes with it.

  • Softer plates conform to the uneven liner and reach further into the valleys between the flutes at kiss impression, which evens out solids.
  • Thicker plates with deep relief give more cushion over rough or uneven board and keep the non-image floor clear of the board.
  • A compressible layer behind the plate, such as a cushion layer on the carrier sheet or a foam mounting tape, absorbs part of the variation in flute height.

The usual objection is that a softer plate will smear fine text. The answer is to choose hardness, relief and screen ruling together for the job, so the plate still holds the text and barcode. Our corrugated flexo plate page covers gauge and hardness, the flexo plate thickness guide explains how gauge and cushion fit the press, and the guides to sleeves and mounting tape and flexo plate mounting cover the layers behind the plate.

For high-graphic boxes the process route often matters more. Die-cut styles print better with off-line die cutting. When direct print cannot reproduce halftones or photographs, print the liner before corrugating or print a label for the panel. Our corrugated preprint vs postprint article compares the two flexo routes.

What to check on incoming board

A second common belief is that washboarding and patchy print are plate or press faults. Many corrugated print defects start in the board itself, so check each lot of board before it goes into the feeder. Mark each item as pass, fail or not checked: flute structure, caliper across the lot, washboarding visible on the unprinted liner, blank length, warp, and whether the board is still warm from the corrugator.

For talks with your board supplier, a list of conditions that suit flexo printing is useful:

Board property Condition that suits flexo
Printing liner weight Typically at least 38 lb per 1,000 sq ft (about 185 g/m²)
Liner surface Smooth finish (supercalendered), flat, no loose fibres, no surface dust
Liner coating A suitable, moderate coating
Colour and brightness Even across the lot
Flute Medium and small flutes, B to N
Medium Good quality, typically at least 24 lb per 1,000 sq ft (about 117 g/m²)
Caliper and moisture To the agreed specification
Washboarding None

For cost reasons no board meets all of these at once. Use the list to agree priorities with the supplier, not to reject every lot. The supplier’s data sheet and your agreed specification decide the grade. The corrugated printing page shows where postprint, preprint and litho-lamination fit.

Corrugated print defects troubleshooting table

Symptom Likely cause Check or fix
Stripes in solids and tints that follow the flutes Washboarding: liner not flat over the flutes, light liner, coarse flute Do not add pressure; check the liner and flute with the board supplier; softer plate and cushion at kiss impression
Sunken areas that do not take ink Leaning, uneven or collapsed flutes Set the lot aside and report it; do not print harder into the low spots
Thinner, weaker board after printing Crushed board from impression or feed roll pressure Reduce impression to kiss; use light pressure on feed rolls or belts
Double feeds or skewed sheets Feed gate not set to the lot’s caliper; too little guiding force Set the gate neither tight nor loose; check caliper across the lot
Short blanks that skew, jam or do not glue Cut short, or warm board shrinking as it cools Let the board reach room temperature and measure again
Feeding problems with bowed or twisted sheets Warp Work around it on the press; report the lot to the board supplier
Patchy solids on rough liner Rough surface, loose fibres, dust Discuss liner finish with the supplier; check plate, anilox and ink together

For ink and press faults such as dirty print or halos, see our guide to flexo printing problems. Bands across the board at a regular interval are covered in barring and gear marks.

FAQ

What is washboarding in corrugated printing?

Washboarding is the flute pattern showing in the print. The liner is not flat over the flutes, so the plate prints harder on the flute tips than between them, and solids and tints show stripes that follow the flutes.

Can more printing pressure fix washboarding?

No. More pressure crushes the board, lowers its caliper and flat crush strength, and the print quality falls. Print at kiss impression and solve washboarding at the board and the plate.

What causes washboarding on corrugated board?

Mainly the board: a liner that is not flat over the flutes, a light liner, coarse flutes and uneven flute structure. Extra impression and a heavy ink film make it worse.

Why are corrugated blanks too short?

Either they were cut short at the corrugator, or the board was still warm and moist and shrank as it cooled. Let the board reach room temperature in the press hall and measure again.

Should corrugated board be printed straight off the corrugator?

It is better to wait. Warm, moist board shrinks as it cools and changes ink transfer and drying, so let it reach room temperature first.

How does the flexo plate affect washboarding?

A softer, thicker plate with a compressible layer behind it conforms to the uneven liner and evens out solids at kiss impression. Choose hardness, relief and screen together so fine text and barcodes still hold.

Fighting flute lines on your box line? Request a quote for corrugated flexo plates with your flute, liner, press, plate gauge and ink system, or ask a technical question.

Disclaimer: the causes and checks on this page are general pressroom practice and for reference only. Board grades are set by your board supplier’s data sheet and your agreed specification; plate gauge and hardness are confirmed in the plate grade’s technical data sheet and the quotation.

About Feng Yan

Feng Yan is a technical engineer at CTPPress with more than 20 years in the printing industry and extensive front-line experience supporting printing plants. Feng specialises in solving the difficult problems printers run into in production.

Talk With Author >>

Start Your Business With Us

Simple Contact Form

Tell us what you need

Request a Quote

Tell us which printing plates or equipment you need, including specifications, quantity and destination. Use the form to send your enquiry.

Aluminium coils and printing plate production equipment
Product Enquiry

Request an Instant Quote

We reply within 24 hours on working days

Product Enquiry
Aluminium coil on an offset plate production line

Send an Enquiry


Product Enquiry