Last updated: November 2026
Quick answer: PS plate dot loss has different causes at each stage. Dots that are not solid after exposure point to dirty glass or film, weak vacuum, poor contact or stray light, then to the developer. Dots smaller than on the film point to over-exposure, scattered light, over-development or thin film. Image that wears off on press points to light, an over-developed plate, strong cleaners, hard tools or high pressure. Check film, frame and developer before you blame the plate.
Key takeaways
- PS plate dot loss shows up after exposure, after development or on press. Where you first see it tells you where to look.
- For dots that are not solid after exposure, check the exposure step first: glass, film, vacuum, the frame blanket and stray light. Then check development.
- For dots smaller than on the film, look at exposure, development and the film. Only one of the nine causes is the plate itself.
- Developer that is too strong, too hot or left too long takes fine dots away, and over-replenishment does the same.
- A plate made from thin film or over-developed will not give its run length. Remake it instead of sending it to press.
Highlight dots are lost after developing. Under the loupe the dots are not solid on the plate, a flat tint looks soft, or the image wears off before the run is finished. This guide sorts these faults by what you see and where to look: exposure, contact, development, handling and the press, with the remedy for each cause. Background faults such as scumming, toning and poor ink take at start-up are covered in a separate article.
Where dots and image are lost
Name the fault and the point where it first appears. Compare the plate with the film under a loupe.
| What you see | When it appears | Where to look |
|---|---|---|
| Dots sometimes not solid | After exposure and development | Exposure: glass, film, vacuum, frame blanket, stray light. Development: concentration, replenishment, temperature, time |
| Soft dots over a large flat tint | After exposure | Film and exposure frame first, then the plate |
| Dots smaller than on the film | After exposure and development | Exposure, development, film, plate |
| Coating partly gone, image missing in places | After development, storage or transport | Storage and handling, operation, the plate |
| Image wears off early, run length short | On press | Plate room and pressroom light, plate making, press chemistry and pressure, paper |
A common belief is that dot loss means the plate is bad. Check the film, the exposure frame and the developer before you blame the plate.
Dots not solid after exposure: contact, glass and film
When the dots are sometimes not solid after exposure, check the exposure step first and development second. On the exposure side, each cause has its own remedy:
- Dust or dirt on the exposure glass. Wipe the glass with a cleaner.
- Vacuum pump system fault, so the vacuum is not enough. Check the vacuum system, for example vacuum hoses that are aged or blocked.
- Dirt, dust or foreign matter on the film. Clean the film or wipe it lightly.
- Film positive montage made badly, for example type stuck too close to a picture. Keep the edges of stripped-in film at least 3 mm away from the image.
- Poor vacuum contact between the film positive and the plate. Check that the film lies tight on the plate everywhere.
- Frame blanket not right. Adjust the rubber blanket of the frame so it is flat and has no wrinkles.
- Stray light on the plate in storage or before exposure. Do not use plates from damaged cartons, and handle plates under yellow safelight from the moment they leave the carton.
For soft dots over a large flat tint, first confirm that the film and the exposure frame are in order, then look at the plate. A base that is not flat enough calls for plates with a flat base, and a poor coating for plates with a matt coating. With plates that have no matt coating, drawing the vacuum several times reduces poor contact.
Our PS plate exposure guide explains the vacuum stages and the grey scale. A plate exposure unit with a two-stage vacuum helps the film lie flat.
Dots smaller than on the film
Look in four places: exposure, development, the film and the plate.
- Exposure. Over-exposure: reduce the exposure time. Scattered light from the light source: adjust the light source, and where a second exposure is given, mask the image areas suitably during it.
- Development. Concentration too high, temperature too high or time too long; see the next section.
- Film. Film dot density not high enough: raise the density of the film. Film dots not solid: check the film output system. Other defects in the film: make a new film.
- Plate. Poor dot reproduction of the plate: choose a plate with good dot reproduction.
Over-exposure burns out fine highlights on a positive plate, so the grey scale check in the exposure guide is the first test here. Change one setting at a time.
Development faults that take dots away
Many operators believe that stronger development gives a cleaner plate. Developer that is too strong, too hot or left too long takes fine dots away. They cause both dots that are not solid and dots that shrink:
| Developer fault | Remedy |
|---|---|
| Concentration too high | Mix the developer at the concentration the maker recommends |
| Replenishment wrong | Adjust the replenishment rate and do not over-replenish |
| Temperature too high | Keep the developer at the temperature the plate needs |
| Time too long | Use the time the maker recommends, and find the right time with a standard dot step wedge |
For our positive PS plate, the data sheet gives a typical developing temperature of 22 to 25 °C and a developing time of 20 to 40 seconds in positive PS developer. Our developer page explains how replenishment keeps the bath stable as plates pass and as the bath ages.
Coating coming off before press
When parts of the coating come off and the image is missing in places, look at storage, operation and the plate.
- Scratches in storage or transport. Carry plates gently and keep the coating away from anything that can scrape it.
- Scratches from weight. Do not stack plates too high.
- Solvent or other chemicals dropped on the plate, or the plate wiped with a cotton cloth. Keep other chemicals away from the plate during exposure and development.
- Developer concentration too high. Adjust the developer to the right ratio.
- The plate surface contaminated in one area before it was coated. Take a new plate and expose it again.
Only the last cause is a plate fault.
Image wearing off on press and short run length
When the image wears off before the run is finished, look at the light in the plate room and pressroom, how the plate was made and treated, and the materials.
- White light falling directly on the plate in the plate room or pressroom. Work under yellow light in the plate room. In the pressroom, keep direct sunlight and incandescent lamps off the plates.
- Stray light during plate making before press, or during printing. Prevent light leaks, and keep finished plates away from light on the way to the pressroom.
- A plate exposed from film that was not dense enough, sent to press anyway. Output the film again.
- An over-developed plate sent to press anyway. Make a new plate that meets the requirements, then put it on press.
- Plate cleaning paste too strong. Use a milder paste.
- Plate cleaner used too often. Wipe the plate with cleaner less often.
- Fountain solution not right. Change to a different fountain solution.
- Pumice sticks or other hard tools used to remove dirt. Never use hard tools on the plate. They destroy the oxide layer.
- Pressure at the impression cylinder too high. Adjust the pressure.
- Paper that sheds heavy dust. Wash the blanket more often. This reduces the effect but does not stop the dusting.
A common belief is that a weak plate can still go to press and hold. A plate made from thin film or over-developed will not give its run length, so remake it instead of sending it to press.
Our positive PS plate gives a typical run length of at least 80,000 impressions unbaked and at least 200,000 impressions baked, under the test conditions on its data sheet. Real run length depends on the press, paper, ink and fountain solution. For longer runs, see printing plate baking. For press-side wear in more detail, see plate wear causes.
PS plate dot loss troubleshooting table and order of checks
| Symptom | Likely cause | Check or fix |
|---|---|---|
| Dots not solid: exposure side | Dust on glass or film, weak vacuum, poor contact, film stripped too close to the image, frame blanket not flat, stray light | Clean glass and film; check vacuum hoses and contact; keep film edges at least 3 mm from the image; flatten the blanket; handle under yellow safelight |
| Dots not solid: development side | Developer too strong, over-replenished, too hot or too long | Correct concentration, replenishment, temperature and time |
| Soft dots over a large flat tint | Film or frame fault; plate base not flat; no matt coating | Confirm film and frame first; draw the vacuum several times; choose a flat, matt plate |
| Dots smaller than on the film | Over-exposure, scattered light, over-development, thin or faulty film | Reduce exposure; adjust the light source; correct the developer; remake the film |
| Coating gone in places | Scratches, stacking weight, chemicals on the plate, strong developer | Handle gently; stack lower; keep chemicals away; adjust the developer |
| Image wears off early on press | White light, thin film or over-developed plate sent to press, strong cleaners, hard tools, high pressure, dusty paper | Control light; remake the plate; use milder cleaners and less often; never use hard tools; adjust pressure; wash the blanket more often |
An order of checks before you change the plate, following the path the plate takes:
- Storage and light. Cartons undamaged, stacks not too high, yellow safelight from opening to development.
- Film. Density, solid dots, no dirt, montage edges clear of the image.
- Exposure frame. Clean glass, a flat blanket, full vacuum and good contact.
- Exposure. A grey scale check, as in the exposure guide.
- Development. Concentration, temperature, time and replenishment against the data sheet.
- Press. Light on the plates, cleaners, fountain solution, tools used on the plate, pressure and paper.
- The plate. Only when the stages above are clear.
If you are deciding whether to stay with film, our CTP vs PS plates guide compares the two routes.
FAQ
Why are highlight dots lost on a PS plate?
Look at over-exposure, scattered light, developer that is too strong, too hot or left too long, and film that is not dense enough. Suspect the plate only after these are clear.
Why are the dots not solid on my PS plate?
Check the exposure step first: dirty glass or film, weak vacuum, poor contact, a frame blanket that is not flat and stray light. Then check the developer.
Can over-development cause dot loss on a PS plate?
Yes. Developer that is too strong, too hot or left too long takes fine dots away. An over-developed plate also gives a shorter run, so remake it.
Why does the image wear off a PS plate on press?
Causes include white or stray light, a plate made from thin film or over-developed, strong or frequent plate cleaners, unsuitable fountain solution, hard tools, high pressure and dusty paper.
How does stray light affect PS plates?
Stray light before exposure can leave dots that are not solid, and white light shortens run length. Handle plates under yellow safelight and keep finished plates away from light.
Does baking help PS plate run length?
On a bakeable plate, yes. Our positive PS plate typically gives at least 80,000 impressions unbaked and at least 200,000 baked, under its test conditions.
Running film and PS plates? Request a quote for positive PS plates with your plate size, gauge and exposure unit, or ask a technical question about a fault you see.
Disclaimer: the causes and remedies on this page are general plate room and pressroom practice and for reference only. Values for our positive PS plate are typical values from its data sheet; set exposure and development on your own equipment and confirm specifications in the quotation.