Last updated: November 2026
Quick answer: The VOC content of ink is the weight of volatile organic compounds per volume of ink. Multiply the VOC share by weight on the safety data sheet by the ink density for lb/gal, then by 119.83 for g/L. For the figure less water, divide by the volume left after the water is taken out. Always state the basis: one water-based ink had 58 g/L as supplied and about 127 g/L less water.
Key takeaways
- The VOC content of ink is the weight of volatile organic compounds in it, given per volume: pounds per gallon (lb/gal) or grams per litre (g/L).
- The same ink gives very different VOC figures on different bases: in one water-based example, 58 g/L as supplied and more than twice that less water. Always state the basis with the number.
- Water-based flexo ink can still contain VOC, such as glycols and glycol ethers. Read the safety data sheet.
- Make-up solvent and washes added at the press also add VOC. Record and count them too.
- The local regulation and the ink supplier’s data sheet decide which definition, which basis and which limit apply.
The customer asks for grams per litre and the sheet is in pounds per gallon. Or the data sheet gives two different VOC figures and you do not know which one to report. Or you have to report VOC but only have the safety data sheet. This guide explains what VOC means for a pressroom and gives you a calculation you can check yourself, with a worked example. It then covers what the press adds and how to cut VOC without losing print quality.
What VOC means in a flexo pressroom
VOC stands for volatile organic compounds: the organic substances in inks, coatings, extenders and washes that evaporate during drying and cleaning. VOC is not only solvent; any organic compound the regulation defines as VOC counts.
- Solvent-based flexo ink. Most of the volatile part is organic solvent, so most of it counts as VOC.
- Water-based flexo ink. The water does not count. Small amounts of glycols, glycol ethers and other organic volatiles do.
- UV flexo ink. It contains no solvent. Nothing evaporates, because the monomers react and stay in the cured film.
Every definition also has exceptions, called exempt compounds. Under the US definition used for the worked example in this guide, water, ammonia and acetone were not counted as VOC. Other regions define VOC and exempt compounds differently; use the definition of the regulation that applies to your plant.
Why VOC content is measured
- Emission reports and permits. In sunlight, VOC reacts with nitrogen oxides and forms ground-level ozone. That is why many regions limit the VOC emissions printing plants release and ask for reports. The local regulation decides what you report, on which basis, and which limit applies.
- Comparing inks. To compare two inks on the same basis, both figures must also use the same definition.
- The workplace. VOC content is an air emission figure, not a health hazard rating. For hazards, read the hazard, protective equipment and first aid parts of the safety data sheet, and train staff before a new ink or wash is used.
How VOC content is expressed
Many people believe an ink has one VOC number. In fact the same ink gives very different VOC figures on different bases, so always state the basis with the number. The weight of VOC stays the same; what changes is the volume you divide it by.
| Basis | Divided by | What the figure tells you |
|---|---|---|
| As supplied (per volume of product) | The whole volume of ink, water included | How much VOC is in a gallon or litre of ink as it comes from the container |
| Less water and exempt solvents | The volume left after the water and exempt compounds are taken out | How much VOC the rest of the ink carries; water no longer dilutes the figure |
| Per volume of solids | The volume of the non-volatile part | How much VOC is released for each gallon of solids that stays on the print |
Units are usually lb/gal or g/L. To convert, 1 lb/gal = 119.83 g/L. Water-based inks contain a lot of water, so their figure less water is much higher than the figure as supplied. A solvent-based ink with no water and no exempt solvents gives the same figure on both bases.
How to calculate VOC content step by step
The method and example below follow US practice published in 1999, using a safety data sheet for a water-based flexo ink; the official method in your region may differ. These steps reproduce every figure on that sheet. You need the ink density, the VOC share by weight, the water share by weight, the density of water and the non-volatile share by volume.
| Figures from the sheet (excerpt) | Value |
|---|---|
| Ink density | 9.00 lb/gal |
| Non-volatile part | 43.82% by weight, 39.32% by volume |
| Volatile part | 56.18% by weight |
| Water | 50.46% by weight; water density 8.33 lb/gal |
| VOC | 5.38% by weight: propylene glycol 3.50%, diethylene glycol monobutyl ether 1.71%, other organic volatiles 0.17% |
| Ammonia | 0.34% by weight, not counted as VOC |
- Decide what counts. List the volatile components and keep only those that are VOC under the definition. Here that is 3.50 + 1.71 + 0.17 = 5.38% by weight. Water and ammonia are left out.
- VOC as supplied. Multiply the VOC share by weight by the ink density: 0.0538 × 9.00 = 0.484 lb/gal. Multiply by 119.83 for g/L: 58.0 g/L. The sheet gives 0.48 lb/gal and 58.03 g/L.
- VOC less water and exempt solvents. First find the water share by volume: water share by weight × ink density ÷ water density = 0.5046 × 9.00 ÷ 8.33 = 0.545. The volume left is 1 − 0.545 = 0.455. Then divide: 0.484 ÷ 0.455 = 1.06 lb/gal, about 127 g/L. Here only the water is taken out. If the ink also contains exempt compounds, find their share by volume the same way, from weight share and density, and subtract it too.
- VOC per volume of solids. Divide the VOC as supplied by the non-volatile share by volume: 0.484 ÷ 0.3932 = 1.23 lb/gal of solids.
- Check against the sheet. Small differences come from rounding. A clear difference means: check the inputs and ask the supplier which basis and definition they used.
The sheet also shows that VOC is only 9.58% of the volatile part by weight; almost all of the rest is water. That is how a water-based ink can show a low VOC figure as supplied and a much higher one less water.
Make-up solvent and washes add to the total
A common belief is that the VOC in the ink as supplied is what the plant emits: “the ink figure is our whole emission”. In fact make-up solvent and washes added at the press also add VOC, so record and count them too.
- Make-up solvent. Solvent-based ink loses solvent during the run and its viscosity rises, so the operator adds solvent. Add make-up solvent only as the ink supplier instructs, and base each addition on a cup reading, not on guesswork. See the Zahn cup viscosity guide.
- Washes and additives. Press, anilox and plate washes count, and so do extenders and slow solvents.
To know what a job really used, run a material balance: weigh the ink and solvent that go into the press and come back out, and count the impressions exactly. Watch every variable and average over several shifts. Multiply the weight of each product used by its VOC share by weight to get the VOC the job brought in. Whether captured or destroyed VOC may be subtracted is for the local regulation to decide.
How the ink system changes VOC
Many printers believe water-based flexo ink contains no VOC. In fact water-based ink can still contain VOC, such as glycols and glycol ethers, so read the safety data sheet. In the worked example, the VOC came from propylene glycol and a glycol ether.
| Ink system | VOC | Check before you change |
|---|---|---|
| Solvent-based | Mature and wets most substrates; VOC is its main drawback | Solvent balance during the run |
| Water-based | Usually lower VOC, but not always zero; glycols and glycol ethers count | On film: treated film and a wetting agent; drying only by evaporation; chrome anilox rolls wear, ceramic suits; pH control |
| UV | No solvent; nothing evaporates | Curing unit, chemical protection for staff, plates that resist UV ink and wash |
A low VOC flexo ink is not automatically a better ink. Do not assume a VOC-free ink will print just as well: inks with all VOC removed have tended to print poorly, so trial any new ink on your press, substrate and plates first. See water-based flexo ink pH and the UV flexo ink guide; see solvent vs water-based flexo ink. On film for flexible packaging, a new ink system affects drying, adhesion and the whole flexographic printing process.
The ink also decides the plate grade: water-wash plates are not for UV inks. The plate room is a separate source of solvent. Water-wash flexo plates remove washout solvent from it; see solvent, water-wash and thermal processing.
Practical ways to reduce VOC
You can change what goes into the pressroom, or treat the exhaust that comes out.
| Action | Effect | Check first |
|---|---|---|
| Change to water-based, high-solids or UV inks | Less VOC per job | Substrate, drying or curing, plate grade, print trial |
| Use low-VOC washes | Cuts the wash share | Compatibility with plates, rollers and anilox |
| Control viscosity with a cup and records | Fewer solvent additions, less ink used | Fixed measuring routine on every unit |
| Print white only to the opacity the job needs | Less ink used | Measure opacity with an instrument, not by eye |
| Keep ink and solvent containers closed, labelled with content and date | Less evaporation in the pressroom | Every container at the press |
| Reuse returned ink; mix waste ink into black or a similar colour | Less waste ink | Check, weigh and seal returned ink |
| Schedule jobs from light to dark colours | Fewer full wash-ups | Job sequence and colour order |
| Solvent recovery, thermal or catalytic oxidation | Treats the exhaust air | Engineering study and local permit |
Carbon adsorption is not widely used in flexo: alcohols and acetates mix with water and can form azeotropes, and acetates can break down into acetic acid, so the solvent is hard to recover.
FAQ
What is the VOC content of ink?
It is the weight of volatile organic compounds per volume of ink, usually in lb/gal or g/L. The figure depends on the basis: as supplied, less water and exempt solvents, or per volume of solids.
How do you calculate VOC in printing ink?
Multiply the VOC share by weight by the ink density for lb/gal as supplied, and by 119.83 for g/L. Less water: divide by the volume share left after the water is taken out. Per solids: divide by the non-volatile share by volume.
Does water-based flexo ink contain VOC?
It can. In the worked example, a water-based flexo ink contained 5.38% VOC by weight, from propylene glycol and a glycol ether. Read the safety data sheet of each ink.
What does VOC less water and exempt solvents mean?
It is the VOC divided by the volume left after the water and exempt compounds are taken out. For a water-based ink it is much higher than the figure as supplied: in the example, 1.06 lb/gal against 0.48 lb/gal.
How do you convert VOC from lb/gal to g/L?
Multiply by 119.83. In the example, 0.484 lb/gal is 58.0 g/L.
How can a flexo printer reduce VOC emissions?
Change to a lower VOC ink system after a print trial, use low-VOC washes, control viscosity with a cup, keep containers closed, schedule jobs from light to dark, and where needed treat the exhaust by solvent recovery or oxidation.
Changing ink system? A different ink can need a different plate grade. Request a quote with your ink system, substrate and press, or ask a technical question. See our flexo plates for the grades we supply.
Disclaimer: general pressroom practice and a worked example from US practice of the late 1990s, for reference only. This page states no legal limit and does not say that any ink complies. The local regulation decides the VOC definition, calculation method and limits; the ink supplier’s data sheet decides each product’s VOC content.